TECHNICAL · 6 min read

Brass Grades Compared: CW614N vs CW617N vs DZR

Three grades cover most of what we make. Here is how to choose between them.

PropertyCW614N (CuZn39Pb3)CW617N (CuZn40Pb2)CW602N (DZR)
Main useTurned parts, inserts, terminalsHot forgings, fittingsDrinking-water fittings
Copper57–59%57–59%61–63%
Lead2.5–3.5%1.6–2.5%1.7–2.8%
Machinability100 (reference)9070
Hot forgeabilityFairExcellentGood
Dezincification resistanceNoNoYes (ISO 6509)
Tensile strength360–480 MPa360–460 MPa280–380 MPa
Relative cost1.001.001.08

How to choose

  • CW614N for anything turned from bar where water contact is not a concern: inserts, terminals, bushes, screws.
  • CW617N for forged parts such as valve bodies, unions and fittings.
  • CW602N DZR wherever the part sits in drinking water or aggressive water. Zinc can leach out of ordinary brass and leave a weak, porous copper shell.

Lead-free options

Where lead limits apply (US SDWA, German UBA list, California AB 1953) we use CW724R (silicon brass) or CW511L. They machine more slowly and cost 15–25% more.